DEV Community

Ray Wang
Ray Wang

Posted on

Girth Seams at 5000 mm: What Actually Changes in the Welding Procedure

A 5000 mm outside diameter is usually presented as a mill capability. In fabrication terms it is a joint: 3000 mm JCOE sections welded end to end. Once the order includes a girth seam, the welding procedure - not the rolling line - is what governs whether the pipe is accepted.

Five things change when a circumferential seam enters the scope.

1. Fit-up becomes the controlling variable

At the girth joint, two independently formed shells meet. Ovality that was acceptable on each section separately can produce a mismatch of 2-3 mm at the joint. On a 6 mm wall, a 2 mm mismatch is a third of the wall thickness, and no procedure can weld that out.

The practical answer is to measure ovality at the pipe ends before fit-up, index the two sections so the high points are 90 degrees apart rather than aligned, and use a hydraulic internal lineup clamp rather than external chain clamps on thin wall.

2. Heat input budget

Austenitic grades have low thermal conductivity and a high expansion coefficient. A girth seam welded at the heat input used for a longitudinal seam will pull the shell out of round, and it will also spend more time in the sensitisation range.

Typically the girth seam runs lower heat input and faster travel than the longitudinal seam, with interpass temperature controlled and measured rather than assumed. Narrow-gap GTAW or plasma with a trailing shield is common at 8-20 mm wall; autogenous GTAW for thin wall.

3. Distortion control

Sequence matters more than technique. Balanced welding around the circumference (opposite quadrants at the same time), back-stepping, and strongbacks where the shell is thin. Root gap and misalignment are recorded, not just corrected.

4. NDT of the girth seam

The girth seam is usually 100% radiographed or ultrasonically tested regardless of the percentage applied to the longitudinal seam. Acceptance levels come from the product specification, and the technique has to match the wall: a heavy-wall radiography setup will wash out thin-wall defects, and a thin-wall setup on 20 mm wall will not penetrate.

5. Documentation

A girth seam means a second WPS and PQR, plus welder qualification for that position and that thickness range. ASME IX or EN ISO 15614-1 qualification, welder performance to EN ISO 9606-1 or ASME IX as applicable, heat input records, and the NDT reports all travel with the mill test certificate.

The inquiry line that avoids the dispute

One sentence in the purchase order settles most of it: whether circumferential seams are permitted, and if so, to which NDT level and with what ovality limit at the joint. Without it, the mill builds to its default and the buyer inspects to an expectation that was never written down.

The route from plate to finished shell is described on the large diameter stainless steel welded pipe page, and the nickel alloy grades that most often run in this size range are set out in these Hastelloy welded pipe grades notes.

Shiwang Pipe manufactures large diameter stainless and special alloy welded pipe: OD 219-5000 mm, wall 3-80 mm, JCOE formed with circumferential seam welding.

Top comments (0)